Lydlinch Bridge: A Tale of Temporary Bridge Construction
Small but mighty, the history and performance of the Callender-Hamilton temporary bridge at Two Fords, Lydlinch, Dorset is impressive.
As early as 1942 the Ministry of Defence was considering outline plans for the D-Day invasion. Where and when the landings would take place were top secret, but the speedy movement of the invasion force to the south coast ports was a common factor to all alternatives. One such route, the A357 through Dorset, Poole Harbour, needed to be improved.
Callender-Hamilton temporary bridge
| Construction date: | Location: | Predicted coating life: |
|---|---|---|
| 1942 | Dorset, England | 120 years (C2) |
At Lydlinch, the picturesque narrow stone bridge over the River Lyden would not withstand the weight of heavy tanks. In 1942 Canadian army engineers erected a temporary galvanized steel Callender-Hamilton bridge alongside the older structure. The tanks and heavy equipment were diverted over the galvanized bridge on their way to Europe.
Temporary Bridge Construction
How a Temporary Bridge Became a Dorset Landmark
The bridge was not intended to be a permanent structure, but has stayed in service having been passed into Dorset County Council’s control after the war. It has carried the road’s eastbound traffic ever since.
We have had no real trouble ensuring that this ‘temporary bridge’ is brought up to the new standard and the bridge was in remarkably good shape
Chief Bridge Engineer
The bridge has seen only minor changes to its original design since it was erected. Timber deck repairs were carried out in 1985 and 2009. The only work of any structural note was that of strengthening the bridge in 1996 to enable it to conform to new standards in order to carry 40t lorries.
At the time Ted Taylor, Dorset’s chief bridge engineer said “We have had no real trouble ensuring that this ‘temporary bridge’ is brought up to the new standard and the bridge was in remarkably good shape”.
In actual fact, the strengthening consisted of bolting ‘T’ sections to the existing transverse deck beams and the addition of some longitudinal beams. The two main trusses were left as they were in 1942. Engineering forethought meant that on a few sections where a lot of cutting and readjustment of design had taken place, the sections were regalvanized.
Beyond Expectations: Inspection of the Temporary Steel Bridge
As a follow-up to an inspection carried out by Galvanizers Association in conjunction with Dorset County Engineers in 1999, the bridge was re-inspected on 14 October 2014 by GA staff with assistance from Dorset County Engineers.
The bridge still looks in very good condition and on first sight the areas that look to have a slightly weary appearance are mostly due to dirt deposits and growth of moss on the steel surfaces.
Coating thickness measurements were taken on steel members chosen at random from both sides of the bridge after wire brushing so as to remove any surface contaminants or build-up of corrosion products.
The members inspected included the main truss diagonals, joining plates and some bolt heads. Average coating thicknesses on the diagonal trusses ranged from 126μm to 167μm. On the plate sections the average thicknesses were 131μm to 136μm. On bolt heads average coating thicknesses ranged from 55μm to 91μm.
(…)the coating can be expected to provide a life well in excess of 100 years, a tribute to the designers and the men who built it.
Despite all that‘s thrown at it, floodwater, mud and grit salt, after 72 years the galvanized exposed members are still in very good condition.
Les Lock, Project Engineer
Enduring the Elements: 72 Years of Galvanized Steel Excellence
Having started life as a temporary steel structure, the Callender-Hamiliton bridge at Two Fords, Lydlinch, is still in fine fettle 72 years after it was first erected. The bridge has now become part of Dorset folklore and it surely can‘t be far off becoming a listed structure.
The galvanized coating has stood the test of time exceptionally well and taking the remaining coating thicknesses into account along-side zinc corrosion data, the coating can be expected to provide a life well in excess of 100 years, a tribute to the designers and the men who built it.
The bridge inspection was carried out with the kind permission and assistance of Dorset County Council with particular thanks to Les Lock, Project Engineer, Bridge Inspections.